© Copyright 1997-2011, Pacific Roller Die Company, Inc. All Rights Reserved.
Designed by:N.Izgi-2011
                                                                           OFF-LINE ULTRASONIC TEST SYSTEM
CONTENTS
1 - ULTRASONIC  TEST  EVALUATION  METHOD 
2 - OFF-LINE WELD TEST
3 - LASER SEAM TRACKING FOR OFF-LINE AND ON-LINE WELD  TEST


1 - ULTRASONIC  TEST  EVALUATION  METHOD 

    
1.1. Weld  Inspection : 
The test is carried out according to the pulse-echo method for longitudinal weld defects and  through-transmission method for transverse weld defects and also for coupling and performance check of the probes. Angle beam probes are used for longitudinal and transverse weld defects.

     1.1.1. Longitudinal Weld Defect :
Two angle beam probes are facing each other and operate in pulse-echo mode for defects and in a through transmission mode for coupling and performance check of the probes.
 
     1.1.2. Transverse Weld Defect :
Two angle beam probes operate in through-transmission mode.  The transmitting probe transmits the sound  beam at an angle of 45 degree to the weld.  If a transverse defect exists, the sound beam is reflected from there and received by the second probe facing the first one.

     1.2. H.A.Z. Defect :
Laminar defects in Heat Affected Zone are detected by immersion straight beam probes.The immersion probes are coupled via water column.The probes operate in pulse-echo mode.The test is performed by means of evaluation between interface echo and first backwall echo.The possible time variation in water column is compensated by the echo start system.

      1.3. Body Lamination :
Two or four twin crystal probes are used in pulse-echo mode for pipes to be inspected for laminations in base metal.
The probes are moved back and forward on pipe body between weld seams by the oscillating device.  The oscillating device is placed after external S.A.W. station on runout of pipe mill.The coupling between probes and pipe surface is supplied by water gap.Lamination can be detected by evaluation gate to be positioned between interface echo and
first backwall echo or between first and second backwall echo.

2 - OFF-LINE WELD TEST

     2.1.Test Principle :
The pipes are carried individually on pipe cart.  The combination of axial movement of the pipe cart and circumferential turning of the pipe on pipe cart passes the pipes according to spiral angle of weld seam through the testing line.
The probes are lowered to the top of the pipe by means of sensor until reaching the set-up distance between pipe surface and probe mechanism.